STAINLESS TOOL STEELS HEAT TREATMENT

AISI
GRADE NAME
ANNEALING
TEMP
°F
TYPICAL
ANN.
HDN.
BRINELL

PREHEAT
TEMP.
°F
AUSTENITIZING
TEMP.
°F
QUENCH
MEDIUM
TEMPERING
TEMP.
°F
TYPICAL
APPLICATION
HARDNESS
HRC


416 416 R 1525 150/180 1450/1500 1750/1850 Oil 500/800 35/40
17Cr-4Ni MOD CRUCIBLE 174 SXR 1900 30/35 HRC NA NA NA 900/1150 33/42
414 MOD MAXEL 2000 1250/1300 ~300 1250 1550 Air 450/750 35/39
17Cr-4Ni MOD CSM 21 1900 30/35 HRC NA NA NA 900/1150 33/42
420 PREM CSM 420XL 1600/1650 192/241 1350/1450 1850/1875 AIR 450/750 49/53
440C CRUCIBLE 440C 1600/1650 217/255 1425 1850/1900 AIR/OIL 400/800 54/58
440C MOD 154 CM 1650 235 1400/1450 1900/2000 AIR/OIL 400/800 58/62
440C MOD +V CPM S60V (440V) 1600/1625 255/277 1500/1550 1850/2050 AIR 300/500 54/58
420 MOD +V CPM S90V (420V) 1600/1650 255/277 1500/1550 1950/2150 AIR/OIL/SALT 400/750 56/58