PLASTICS TOOLING MATERIALS CHEMISTRIES & PROPERTIES
|
|
|
AISI |
GRADE NAME |
C |
Cr |
V |
Mo |
OTHER |
WEAR RESISTANCE |
TOUGHNESS |
POLISHABILITY |
|
![](plasticsgifs/conventional.gif) |
A2 |
AIRKOOL |
1.00 |
5.25 |
0.25 |
1.10 |
|
|
|
|
A6 |
CSM 6 |
0.70 |
1.00 |
|
1.35 |
2.00 Mn |
|
|
|
D2 |
AIRDI 150 |
1.55 |
11.50 |
0.80 |
0.90 |
|
|
|
|
|
CRU-WEAR |
1.10 |
7.50 |
2.40 |
1.60 |
1.15W |
|
|
|
H13 |
NU-DIE V |
0.40 |
5.20 |
0.95 |
1.30 |
|
|
|
|
H13 PREM |
NU-DIE XL |
0.40 |
5.20 |
0.95 |
1.30 |
0.005 max S |
|
|
|
|
CRU 161 |
0.50 |
5.00 |
1.10 |
1.60 |
|
|
|
|
H13 MOD |
CPM NU-DIE EZ |
0.36 |
5.50 |
0.85 |
1.60 |
0.17 S |
|
|
|
|
KAPSTAR |
0.12 |
0.50 |
0.10 |
0.25 |
4 Ni,1 Al,1.5 Mn,0.10 S |
|
|
|
P20 |
CSM 2 |
0.35 |
1.70 |
|
0.40 |
|
|
|
|
S7 |
CRUCIBLE S7 |
0.55 |
3.25 |
|
1.40 |
|
|
|
|
S7 PREM |
CRUCIBLE S7 XL |
0.55 |
3.25 |
|
1.40 |
0.005 max S |
|
|
|
|
![](plasticsgifs/stainless.gif) |
17Cr-4Ni MOD |
CSM 21(a) |
0.02 |
15.00 |
|
0.20 |
3.50 Cu, 4.75 Ni |
|
|
|
420 PREM |
CSM 420XL |
0.38 |
13.60 |
0.30 |
|
|
|
|
|
440C |
CRUCIBLE 440 C |
1.00 |
17.50 |
|
0.50 |
|
|
|
|
420 MOD+V |
CPM S90V (420V) |
2.30 |
14.00 |
9.00 |
1.00 |
|
|
|
|
414 MOD |
MAXEL 2000 |
0.03 |
12.50 |
|
0.30 |
2.75 Ni, 0.12 S |
|
|
|
|
![](plasticsgifs/cpm.gif) |
|
CPM 3V |
0.80 |
7.50 |
2.75 |
1.30 |
|
|
|
|
|
CPM 9V(b) |
1.80 |
5.25 |
9.00 |
1.30 |
|
|
|
|
A11 |
CPM 10V |
2.45 |
5.25 |
9.75 |
1.30 |
|
|
|
|
|
CPM 15V |
3.40 |
5.25 |
14.50 |
1.30 |
|
|
|
|
M4 |
CPM M4HC(HS) |
1.40 |
4.00 |
4.00 |
5.25 |
5.50 W, 0.06(0.22) S |
|
|
|
420 MOD+V |
CPM S90V (420V) |
2.30 |
14.00 |
9.00 |
1.00 |
|
|
|
|
|
|
4140 MOD + Al |
NITRIDING 135 MOD |
0.40 |
1.60 |
|
0.35 |
1.15 Al (c) |
|
|
|
|
4150 MOD |
HOLDER BLOCK |
0.50 |
0.65 |
|
0.18 |
0.08 S |
|
|
|
|
(a) CSM 21 @H1100 HRC 35, (b) CPM 9V @ HRC 50, (c) Nitrided
|
|